Installation Guide
01
Precision Cutting
Cut the pipe at a 90° angle using sharp PPRC cutters. Ensure the edges are clean, dry, and free from burrs.
02
Fusion Heating
Heat both pipe and fitting simultaneously on the welding machine at 260°C. Do not rotate during heating.
03
Seamless Joining
Push the heated pipe into the fitting without twisting. Align immediately for a permanent molecular bond.
04
Stabilization
Hold the joint firmly during the cooling phase. Allow the connection to stabilize before applying pressure.
Fusion Welding Parameters
(Based on 260°C Welding Temperature)
| Diameter (mm) | Heating Time (sec) | Joining Time (sec) | Cooling Time (min) |
|---|---|---|---|
| 20 mm | 5 | 4 | 2 |
| 25 mm | 7 | 4 | 2 |
| 32 mm | 8 | 6 | 4 |
| 40 mm | 12 | 6 | 4 |
| 50 mm | 18 | 6 | 4 |
| 63 mm | 24 | 8 | 6 |
Engineer's Assurance
At Al Karam Industry, we recommend using only high-quality welding machines calibrated to 260°C. Our 100% virgin raw material is optimized for molecular fusion, ensuring that the joint becomes the strongest part of your entire piping system.